The carbon black was crushed into 325 mesh chromium powder with electrolytic chromium at the ratio of 13.5% ~ 64% (more than the theoretical carbon amount of 11.33%), and then was used as raw material after dry mixing with ball mill. Add 1% ~ 3% stearic acid as lubricant for molding. With 1 T/cm2 or more pressure molding. The pressurized molding powder is put into the graphite plate or crucible, using Taman furnace or induction heating furnace, in the hydrogen flow (hydrogen dew point at -35℃ or so), heated to 1500 ~ 1700℃, and keep 1h, so that the chromium carbonization reaction, chromium carbide, after cooling, chromium carbide. Its reaction equation is as follows:
3Cr + 2C → Cr3C2